In short
- Brassware finishes are processes, not colours: electroplated chrome, vacuum-deposited PVD, powder coating or lacquer. The process sets the wear, the cleaning limits and the repair route.
- PVD is harder than decorative chrome plating and holds a brushed or black colour, but the palette is narrower and recoating happens at the factory, not on site.
- Ask for measured coating thickness in micrometres and a salt spray result naming the part, the hours and the pass criterion. Without those, two finish claims cannot be compared.
A brassware finish is the surface layer on a tap, shower fitting or accessory body, produced by electroplating, physical vapour deposition (PVD), powder coating or lacquer. The layer is thin, the process behind it is specific, and the colour name in the catalogue describes neither the thickness nor the method.
That matters because the finish is where most bathroom complaints land. A dripping tap is a cartridge; a tap gone cloudy at the spout or pale at the lever after two years of cleaning is a finish failure, and the remedy is a replacement part, not a polish. The purchase decision is which process the building can maintain.
01Four processes, four different failure modes
The four routes are applied in four different ways, and each leaves a different weak point. Chrome is electroplated in a bath. PVD is deposited in a vacuum. Powder coat is sprayed as a dry polymer and cured in an oven. Lacquer is a film that dries over polished metal. Colour names sit on top of those processes and describe none of them.
| Finish | Process | Typical substrate | Colour range | What fails first |
|---|---|---|---|---|
| Chrome plating | Electroplated copper, nickel, then chromium | Brass; sometimes zinc alloy | Bright chrome | Cloudy or pitted patches at exposed nickel |
| PVD | Metal vapourised and deposited in a vacuum | Brass, stainless steel | Brushed nickel, gunmetal, black, gold tones | Marks at the lever; no local repair |
| Powder coat | Dry polymer sprayed, cured at 180–200 °C | Aluminium, steel | RAL references, matte and texture | Chipping at edges; lifting once water is beneath |
| Lacquer | Clear or tinted organic film over polished metal | Brass | Clear over polished brass, or tinted | Wear at touch points; yellowing under UV |
The table describes process families, not products. Thickness, cure schedule and colour reference must come from the supplier.
Wear shows first where hands, water and cloths arrive: the lever, the aerator, the base of the spout and the edge of a wall plate. Look there on a sample, not at the middle of a spout.
Decision rule: name the process in the schedule, not the colour alone. 'Matte black, PVD on brass' and 'matte black, powder coat on aluminium' are different line items, and a quote that answers only the colour has not answered the finish question.
02Chrome plating: three layers, one working barrier
Chrome plating is a sequence. A decorative system deposits copper to level the surface, nickel to provide the corrosion barrier and the depth of colour, then chromium for the hard, tarnish-resistant face. Three layers, and the buyer usually treats the third as the whole finish.
The chromium layer is usually less than a micrometre thick, a micrometre being 0.001 mm. The nickel beneath it carries several times that thickness. A 0.2 mm scratch crosses the entire coating system and lands in the brass, which is why a deep mark on a chrome tap blooms into a dark patch instead of polishing out.
EN 248 is the European specification for electrodeposited nickel-chromium coatings on sanitary tapware; it sets minimum thicknesses and describes the corrosion test. EN 817 covers the mixer as a mechanical product. Ask for the measured copper, nickel and chromium thicknesses, in micrometres, on the part being supplied, and the laboratory that measured them. Ask too about the aerator thread, the waste and any drilled edge, where plating is thin or broken and no photograph shows it.
Decision rule: for a hotel, a coastal site or any building with a cleaning contractor, require the EN 248 thickness values for the supplied part and a salt spray report that names it. For a single domestic bathroom, require the cleaning instruction and the spare-parts route.
Catalogue reference: sanitaryware and tap ranges — models, dimensions and finishes for the directions discussed above.
03PVD buys hardness and gives up palette
PVD, physical vapour deposition, happens in a vacuum: metal is vapourised and condenses onto the part as a film measured in fractions of a micrometre. Being deposited rather than grown in a bath, it can be harder than electroplated chromium, and it holds colours plating cannot reach.
The colour list is where buyers get caught. PVD reaches brushed nickel, gunmetal, deep black and gold tones, but not the full RAL range, and a colour approved on one batch is not repeated automatically on the next. The film is hard, not immune: grit under a cloth still marks it.
A marked PVD part is stripped and recoated at the factory. There is no site repair that matches, which turns spares into a specification item. For 120 hotel bathrooms, a 5–10% allowance is 6 to 12 additional lever sets, ordered with the batch.
Decision rule: wherever more than one bathroom is being fitted out, order the spare allowance from the same batch and approve the colour on a physical sample under the light source the building will use.
04Powder coat is a film, and a film has an edge
Powder coating is dry. A polymer powder is sprayed onto a grounded metal part, usually aluminium, and cured in an oven at roughly 180–200 °C. The film is tens of micrometres thick, far thicker than a plating, and that thickness is both the appeal and the problem.
The appeal is colour: RAL references, matte and textured surfaces, and consistency across a large order. The problem is the edge. A thick film has to wrap a machined rim, a thread or a cut-out, and those are where it thins, chips or lifts. Once water sits under a chip, an aluminium body corrodes and the coating peels.
Powder coat also signals a different body. It is most often used on aluminium or zinc alloy, lighter than brass; brass runs at about 8.4–8.7 g/cm³, so 100 cm³ of brass weighs roughly 850 g. A powder-coated aluminium tap and a chrome-plated brass tap are not one product in two colours.
Decision rule: for powder coat, specify the colour reference and gloss level, the substrate alloy, the film thickness in micrometres and the touch-up policy, and record that a touch-up pen is cosmetic rather than a repair.
05Salt spray hours mean nothing on their own
Salt spray is the test most often quoted and least often comparable. ISO 9227 neutral salt spray runs at 35 °C with a 5% sodium chloride solution, about 50 g/L, and a data sheet then reports hours: 24, 48, 96 or more.
Four details decide whether two hour counts can be compared.
| Detail | Reported as | Why it changes the answer |
|---|---|---|
| Part tested | Coupon or finished component | A threaded spout has edges a flat coupon does not |
| Coating thickness | Micrometres, measured on that part | Resistance follows thickness, not colour |
| Pass criterion | Hours to red rust, blister or adhesion loss | Different end points give different hour counts |
| Scribe | Scribed or unscribed sample | A scribed sample tests creep from a damage site |
A 96-hour coupon result and a 48-hour spout result are not the same claim, even when both cite ISO 9227.
Decision rule: compare hours only when the standard, the part, the thickness and the pass criterion match. When one quote cites a coupon and another cites the finished spout, ask both for the spout.
06Four agents strip a finish, and three arrive with a cloth
- Limescale and descaler. Hard water leaves carbonate at the spout and aerator, and the instinct is an acid descaler. Repeated acid contact attacks the chromium, then the nickel; the result is a dull patch or a pitted ring, not a chip.
- Chlorine. Bleach and chlorine-releasing cleaners appear in most tap makers' exclusions, and a bathroom cleaned daily holds a concentration at the spout base between wipes.
- Abrasion at the touch point. Grit on a cloth, a scouring pad or a ring. This is where PVD earns its place and where a lacquer shows its age first.
- Installation damage. A wrench on a finished surface, a screwdriver slip at the wall plate, adhesive left to cure on the body. Most marks found at handover were made by the installer.
Do the arithmetic before dismissing cleaning. A basin tap wiped twice a day for ten years takes about 7,300 contacts with cloth and cleaner. The finish that survives is the one whose cleaning instruction was followed, not the one with the longest salt spray number.
Decision rule: put the cleaning instruction into the handover pack and the housekeeping schedule, and make the supplier state the tolerated pH range in writing before the order is placed.
07The finish schedule and the RFQ clause
A finish schedule that survives a change of supplier carries five lines per item: process, substrate, colour reference, measured thickness and test evidence. Decision rule: freeze those five before any price is compared.
- Name the process and substrate: 'PVD on brass, brushed, colour reference X', 'chrome plating to EN 248 on brass', 'polyester powder coat on aluminium, RAL 9005, matte'.
- Fix the colour on a physical sample approved under a named light source, and keep one approved sample on site.
- Require measured coating thickness in micrometres for the supplied part, and name the method.
- Require corrosion evidence to ISO 9227 with hours, part, thickness, pass criterion and scribe condition.
- State the cleaning limits: permitted cleaner types, prohibited actives, and the pH range confirmed by the supplier.
- Set the spare allowance from the same batch, and the colour-match rule for later deliveries.
A clause to paste into the RFQ: 'Brassware shall be [process] on [substrate], colour [reference], approved on sample [date]. Coating thickness shall be measured on the supplied part and reported in micrometres; plated parts shall meet EN 248. Corrosion resistance shall be evidenced to ISO 9227 NSS with hours, part, thickness and pass criterion stated. The supplier shall provide a cleaning instruction naming prohibited actives and the tolerated pH range, and shall supply [n] spare sets from the same batch.'
On arrival, unwrap two pieces and look at the aerator thread, the underside of the lever and the wall plate edge under raking light. Photograph the batch label against the delivery note. A defect found at handover is a replacement; the same defect found after installation is an argument.
What your RFQ should state
- Process and substrate per item: 'PVD on brass, brushed' or 'polyester powder coat on aluminium, RAL 9005, matte', not a colour name alone.
- Measured copper, nickel and chromium thickness in micrometres to EN 248 for plated parts, with the method named.
- Corrosion evidence to ISO 9227 NSS with hours, the part tested, the thickness on that part, the pass criterion and the scribe condition.
- Colour approved on a physical sample under a named light source, with one approved sample retained on site.
- The supplier's written cleaning instruction, naming prohibited actives and the pH range the finish tolerates.
- Spare levers, spouts or handles ordered from the same production batch, at 5–10% of the installed count.
- A definition of a finish defect at handover, with the inspection light and viewing distance stated.
Where this guidance stops
- This article describes processes and the evidence behind them, not products. Two chrome taps from different factories can differ in nickel thickness, adhesion and colour control.
- A photograph cannot show coating thickness, adhesion or the condition of a thread. Those need a measurement report and a physical sample.
- Salt spray is a laboratory test with a fixed chloride load. A real bathroom adds descalers, abrasion and drying cycles that no hour count models.
- The standards cited are European. Local approval for materials in contact with drinking water differs by market and is not covered here.
- Foshan Supply coordinates sourcing, sampling and inspection. We do not plate, test, certify or warrant a finish; the supplier's declared data and the agreed inspection scope govern.
Questions buyers ask
Is PVD better than chrome plating on a tap?
PVD is harder, so it resists abrasion at a lever better than decorative chrome, and it holds dark and brushed colours that plating cannot. Chrome remains the reference for a bright finish and is easier to have re-plated locally. Choose PVD for a dark or brushed high-touch fitting; chrome where a bright finish and a local repair route matter.
How thick should a chrome plating be?
Ask for the measured copper, nickel and chromium thicknesses in micrometres, to EN 248, for the part being supplied. The chromium layer is usually under a micrometre and does the appearance work; the nickel beneath is several times thicker and does the corrosion work. A 'chrome plated' claim without those figures cannot be checked.
Does powder coating last on a bathroom tap?
It can, on an aluminium body with a well-wrapped film, and it offers colours PVD cannot. The risk is the edge: threads, cut-outs and machined rims are where the film thins, and water under a chip lifts the coating. Specify film thickness, the cure schedule and the alloy, and accept that a touch-up pen is cosmetic.
How many hours of salt spray should a tap finish pass?
There is no single number, because hours only compare when the standard, the part, the coating thickness and the pass criterion match. A 96-hour coupon result and a 24-hour spout result describe different tests. Ask for the report and read the end point: first red rust, blistering or adhesion loss.
Can a scratched tap finish be repaired?
A plated surface can sometimes be re-polished or re-plated, and a powder-coated part touched up cosmetically, but neither restores the original coating. A PVD film is stripped and recoated at the factory. On a project the practical answer is a spare set from the same batch, which is why the allowance belongs in the RFQ.
Which finish suits a brushed brass look?
A brushed brass look is usually a PVD film over brass or stainless steel, or a lacquered polished brass. The PVD version holds colour under cleaning and abrasion; the lacquered version can be re-lacquered but wears at touch points and may yellow. Ask which one is quoted before approving the sample.
What should a hotel specify for 120 bathrooms?
One process, one substrate, one colour reference and one batch, with a 5–10% spare allowance — 6 to 12 extra lever sets — ordered at the same time. Add measured EN 248 thicknesses, ISO 9227 evidence with its pass criterion, and the cleaning instruction. Consistency across 120 rooms is a batch and spares problem before it is a finish problem.
Sources
- EN 248 — Sanitary tapware: general specification for electrodeposited coatings of Ni-Cr — European Committee for Standardization
- EN 817 — Sanitary tapware: mechanical mixers, general technical specification — European Committee for Standardization
- EN 200 — Sanitary tapware: single taps and combination taps, PN 10 — European Committee for Standardization
- ISO 9227 — Corrosion tests in artificial atmospheres: salt spray tests — International Organization for Standardization
- ISO 2409 — Paints and varnishes: cross-cut test — International Organization for Standardization
- EN 14688 — Sanitary appliances: wash basins, functional requirements and test methods — European Committee for Standardization
- EN 14428 — Shower enclosures: functional requirements and test methods — European Committee for Standardization
Pages related to this guide
How this guide was checked
- Written from the public catalogue, the standards and regulator pages listed under Sources, and the process records described on the services page.
- Catalogue references and model details were checked on 2026-11-05; 7 primary sources are linked above.
- No supplier paid for placement. No price on this page is an offer; ranges are planning references and must be confirmed in a quotation.